XRD, TGA and TMA Charts (No.041)

No.NameSampling dateVein or depositMining placeMining companySampling placeGrade or sort
041USDX_22ANovember 15,1983Sarayama V.DenbeekobaUeda TohsekiSite of rock massTranslucent quartz ?

Colors of the milled samples
XYZWhiteness (Hunter)LabWhiteness (Lab)
77.7078.7974.4163.0688.760.9112.4383.22

Chemical compositions (wt%)
SiO2Al2O3Fe2O3TiO2CaOMgONa2OK2OIg.loss
79.5614.170.550.010.060.130.122.752.36


Mineral compositions (wt%)
Q : QuartzM : SericiteK : Kaolin mineralF : FeldsparC : CalciteS : Siderite
56.2832.5710.450.690.010.00


Results of TGA and Colors of the Powder Samples after Measuring
The conditions for TGA were sample weight : about 180mg, heating rate : 20°C/min, ended temperature : 1000°C.
LT : Total weight loss, L400 : Weight loss of 400-1000°C.
LT (wt%)L400 (wt%)XYZWhiteness (Hunter)LabWhiteness (Lab)
2.852.2172.9371.5365.9455.8884.585.9112.9878.99


Results of TMA and Colors of the Sintered Samples after Measuring
The conditions for TMA were compaction pressure : 250MPa, pellet diameter : 10mm, thickness : about 3mm, heating rate : 10°C/min, loading : 10g.
W10 : Contents of particles larger than 10µm, SMax : Maximum shrinkage, T0 : Temperature at the maximum shrinkage, T5 : Temperature at the expansion coefficient becomes 0.0005/°C, TS5 : Temperature rectified using the correlative equation, TSK : Nominal temperature equivalent to its SK.
W10
(wt%)
SMax
(%)
T0
(°C)
T5
(°C)
TS5
(°C)
TSK
(°C)
SKXYZW
(Hunter)
LabW
(Lab)
38.98.9614251437143815852660.2661.7866.5356.3878.60-0.704.8478.05
Back to the list of vein or depositBack to the list of grade or sort