Kyushu / Name of sample: KO-5

No.DistrictName of Pyroclastic DepositeAge
048Kanoya, Kagoshima Pref.Aira-Ohsumi pumice flow16,000-23,000

Particle Size Distribution (wt%).
-0.038mm-0.075mm-0.15mm-0.3mm-0.6mm-1.18mm-2.36mm-4.75mm
8.015.930.948.160.270.079.886.6


Microphotographs of glass particles
(size: 0.15-0.3mm).

X-ray powder diffraction pattern
(F: feldspar, Q: quartz).

Chemical Compositions and Content of Volcanic Glass (wt%).
SiO2Al2O3Fe2O3TiO2CaOMgONa2OK2OIg.lossTotalContent of Volcanic Glass
70.3613.162.480.122.580.623.202.953.4998.9666.39


DTG pattern of separated volcanic glass.
Chemical Compositions of Separated Vocanic Glass (wt%).
SiO2Al2O3Fe2O3TiO2CaOMgONa2OK2OIg.lossTotal
73.6812.381.960.161.470.332.962.723.3398.99